ASA
Outdoor parts: signs, housings, mounts, anything that lives in the sun and rain.
Values from the Bambu Lab ASA, Technical Data Sheet V3.0. Open the original PDF ↗
- Softens at
- 100 °C
- Strength, flat
- 37 MPa
- Strength, upright
- 31 MPa
- Water uptake
- 0.45%
About this grade
Bambu ASA is a highly durable material with exceptional UV, weather, mechanical and thermal resistance. It is ideal for outdoor models such as plant signs, mailboxes and wind vanes, and for structural parts with long-term exposure to outdoor conditions.
Not the best choice for
Contact with some solvents, oils and greases.
Jet black, Bone white, Slate grey
Physical properties
| Property | Test | Value |
|---|---|---|
| Density | ISO 1183 | 1.05 g/cm³ |
| Melting temperature | DSC, 10 °C/min | 210 °C |
| Vicat softening temperature | ISO 306 | 106 °C |
| Heat deflection temperature | ISO 75, 1.8 MPa | 92 °C |
| Heat deflection temperature | ISO 75, 0.45 MPa | 100 °C |
| Saturated water absorption | 25 °C, 55% RH | 0.45% |
Mechanical properties
| Property | Test | Printed flat (X-Y) | Printed upright (Z) |
|---|---|---|---|
| Young’s modulus | ISO 527 | 2450 ± 270 MPa | 2120 ± 260 MPa |
| Tensile strength | ISO 527 | 37 ± 3 MPa | 31 ± 4 MPa |
| Elongation at break | ISO 527 | 9.2 ± 1.4% | 4.6 ± 0.8% |
| Bending modulus | ISO 178 | 1920 ± 130 MPa | 1650 ± 120 MPa |
| Bending strength | ISO 178 | 65 ± 5 MPa | 40 ± 3 MPa |
| Impact strength | ISO 179 | 41.0 ± 2.3 kJ/m² | 4.9 ± 0.6 kJ/m² |
| Impact strength, notched | ISO 179 | 19.6 ± 1.8 kJ/m² | – |
Chemical resistance
| Acids | Resistant |
|---|---|
| Alkalis | Resistant |
| Organic solvents | Not resistant to some organic solvents |
| Oil and grease | Not resistant to some kinds of oil and grease |
| Flammability | Flammable |
Manufacturer's print settings
| Nozzle sizes | 0.2, 0.4, 0.6, 0.8 mm |
|---|---|
| Nozzle temperature | 240–270 °C |
| Bed temperature | 80–100 °C |
| Chamber temperature | 45–60 °C |
| Drying | 80 °C for 8 h |
| Max overhang angle | about 70° |
| Max bridging length | about 40 mm |
How the test bars were made: Printed at 260 °C nozzle, 80 °C bed, 200 mm/s and 100% infill, then annealed and dried at 80 °C for 12 h before testing. These are typical values for solid test bars, for comparing materials. A real part's strength also depends on its shape, infill and which way it was printed. Source: Bambu Lab ASA, Technical Data Sheet V3.0.