PETG
Long-lasting everyday parts: brackets, clips, enclosures, snap fits.
Values from the Bambu Lab PETG HF, Technical Data Sheet V1.0. Open the original PDF ↗
- Softens at
- 69 °C
- Strength, flat
- 34 MPa
- Strength, upright
- 23 MPa
- Water uptake
- 0.40%
About this grade
Bambu PETG HF is a PETG optimised for high-speed printing, with a matte finish. It offers greater durability and toughness than PLA and suits long-lasting items.
Not the best choice for
Parts that get hotter than about 60 °C.
Cobalt, Jet black, Bone white, Slate grey, Molto orange, Clear
Physical properties
| Property | Test | Value |
|---|---|---|
| Density | ISO 1183 | 1.28 g/cm³ |
| Melting temperature | DSC, 10 °C/min | 214 °C |
| Glass transition temperature | DSC, 10 °C/min | 66 °C |
| Vicat softening temperature | ISO 306 | 70 °C |
| Heat deflection temperature | ISO 75, 1.8 MPa | 62 °C |
| Heat deflection temperature | ISO 75, 0.45 MPa | 69 °C |
| Saturated water absorption | 25 °C, 55% RH | 0.40% |
Mechanical properties
| Property | Test | Printed flat (X-Y) | Printed upright (Z) |
|---|---|---|---|
| Young’s modulus | ISO 527 | 1810 ± 190 MPa | 1540 ± 130 MPa |
| Tensile strength | ISO 527 | 34 ± 4 MPa | 23 ± 4 MPa |
| Elongation at break | ISO 527 | 8.6 ± 1.2% | 5.1 ± 0.8% |
| Bending modulus | ISO 178 | 2050 ± 120 MPa | 1810 ± 140 MPa |
| Bending strength | ISO 178 | 64 ± 3 MPa | 48 ± 4 MPa |
| Impact strength | ISO 179 | 31.5 ± 2.2 kJ/m² | 10.6 ± 1.2 kJ/m² |
| Impact strength, notched | ISO 179 | 6.2 ± 1.8 kJ/m² | – |
Chemical resistance
| Acids | Not resistant |
|---|---|
| Alkalis | Not resistant |
| Organic solvents | Not resistant to some organic solvents |
| Oil and grease | Resistant to most kinds of oil and grease |
| Flammability | Flammable |
Manufacturer's print settings
| Nozzle sizes | 0.2, 0.4, 0.6, 0.8 mm |
|---|---|
| Nozzle temperature | 230–260 °C |
| Bed temperature | 65–75 °C |
| Chamber temperature | 35–50 °C |
| Drying | 65 °C for 8 h |
| Max overhang angle | about 70° |
| Max bridging length | about 30 mm |
How the test bars were made: Printed at 255 °C nozzle, 70 °C bed, 200 mm/s and 100% infill, then annealed and dried at 75 °C for 8 h before testing. These are typical values for solid test bars, for comparing materials. A real part's strength also depends on its shape, infill and which way it was printed. Source: Bambu Lab PETG HF, Technical Data Sheet V1.0.