Values from the Bambu Lab TPU 95A HF, Technical Data Sheet V1.0. Open the original PDF ↗

Softens at
Flexible
Strength, flat
27.3 MPa
Strength, upright
22.3 MPa
Water uptake
1.08%

About this grade

Bambu TPU 95A HF is a TPU optimised for high-speed printing. It keeps the interlayer adhesion, impact resistance, flexibility and cold-temperature resilience of standard TPU 95A.

Not the best choice for

Parts that must stay rigid. It stretches to more than six times its length before it breaks.

Jet black, Bone white, Molto orange

Physical properties

PropertyTestValue
DensityISO 11831.22 g/cm³
Melting temperatureDSC, 10 °C/min183 °C
Heat deflection temperatureISO 75Not applicable
Saturated water absorption25 °C, 55% RH1.08%

Mechanical properties

PropertyTestPrinted flat (X-Y)Printed upright (Z)
Young’s modulusISO 5279.8 ± 0.7 MPa7.4 ± 0.6 MPa
Tensile strengthISO 52727.3 ± 0.8 MPa22.3 ± 0.6 MPa
Elongation at breakISO 527over 650%over 480%
Impact strengthISO 179123.2 kJ/m²86.3 kJ/m²

Chemical resistance

AcidsNot resistant
AlkalisNot resistant
Organic solventsNot resistant to some organic solvents
Oil and greaseResistant to most kinds of oil and grease
FlammabilityFlammable

Manufacturer's print settings

Nozzle sizes0.4, 0.6, 0.8 mm
Nozzle temperature220–240 °C
Bed temperature30–35 °C
Chamber temperature25–45 °C
Drying70 °C for 8 h
Max overhang angleabout 55°
Max bridging length20 mm

How the test bars were made: Printed at 230 °C nozzle, 35 °C bed, 140 mm/s and 100% infill, then annealed and dried at 70 °C for 12 h before testing. These are typical values for solid test bars, for comparing materials. A real part's strength also depends on its shape, infill and which way it was printed. Source: Bambu Lab TPU 95A HF, Technical Data Sheet V1.0.